ASTM testing results

Sandy Creek

Material Type: Quartzitic Sandstone

Material Class: Metamorphic

ASTM C97-96

Dry Density

158.7 pcf

ASTM C97-96

Bulk Specific Gravity

2.54

ASTM C97-96

Absorption

0.5%

ASTM C99-87

Modulus of Rupture

1,850 psi

ASTM C170-90

Compressive Strength

17,700 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

ASTM C241-90

Abrasion Resistance

63.8

Mohs Hardness

6-7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

0.873

0.688

Polished

0.558

0.473

Thermal

0.896

0.783

Tapestry

0.889

0.722

Bush Hammer

1.000

1.050


Highland Brown

Material Type: Quartzitic Sandstone

Material Class: Metamorphic

ASTM C97-96

Dry Density

158.7 pcf

ASTM C97-96

Bulk Specific Gravity

2.54

ASTM C97-96

Absorption

0.5%

ASTM C99-87

Modulus of Rupture

1,850 psi

ASTM C170-90

Compressive Strength

17,700 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

ASTM C241-90

Abrasion Resistance

63.8

Mohs Hardness

6-7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

0.873

0.688

Polished

0.558

0.473

Thermal

0.896

0.783

Tapestry

0.889

0.722

Bush Hammer

1.000

1.050


Chestnut

Material Type: Quartzitic Sandstone

Material Class: Metamorphic

ASTM C97-96

Dry Density

158.7 pcf

ASTM C97-96

Bulk Specific Gravity

2.54

ASTM C97-96

Absorption

0.5%

ASTM C99-87

Modulus of Rupture

1,850 psi

ASTM C170-90

Compressive Strength

17,700 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

ASTM C241-90

Abrasion Resistance

63.8

Mohs Hardness

6-7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

0.873

0.688

Polished

0.558

0.473

Thermal

0.896

0.783

Tapestry

0.889

0.722

Bush Hammer

1.000

1.050


Glacier Bay

Material Type: Quartzitic Sandstone

Material Class: Metamorphic

ASTM C97-96

Dry Density

158.7 pcf

ASTM C97-96

Bulk Specific Gravity

2.54

ASTM C97-96

Absorption

0.5%

ASTM C99-87

Modulus of Rupture

1,850 psi

ASTM C170-90

Compressive Strength

17,700 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

ASTM C241-90

Abrasion Resistance

63.8

Mohs Hardness

6-7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

0.873

0.688

Polished

0.558

0.473

Thermal

0.896

0.783

Tapestry

0.889

0.722

Bush Hammer

1.000

1.050


Cambrian Cream

Material Type: Quartzitic Sandstone

Material Class: Metamorphic

ASTM C97-96

Dry Density

158.7 pcf

ASTM C97-96

Bulk Specific Gravity

2.54

ASTM C97-96

Absorption

0.5%

ASTM C99-87

Modulus of Rupture

1,850 psi

ASTM C170-90

Compressive Strength

17,700 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

ASTM C241-90

Abrasion Resistance

63.8

Mohs Hardness

6-7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

0.873

0.688

Polished

0.558

0.473

Thermal

0.896

0.783

Tapestry

0.889

0.722

Bush Hammer

1.000

1.050


Aqua Blue

Material Type: Granitic Gneiss

Material Class: Metamorphic

ASTM C97-96

Dry Density

189.3 pcf

ASTM C97-96

Bulk Specific Gravity

3.03

ASTM C97-96

Absorption

0.0%

ASTM C293-94

Modulus of Rupture

2,910 psi

ASTM C170-90

Compressive Strength

22,710 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

Mohs Hardness

7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

.728

.733

Polished

.594

.539

Thermal

.859

.754

Tapestry

.911

.846

Bush Hammer

.800

.900


Aqua Grantique

Material Type: Granitic Gneiss

Material Class: Metamorphic

ASTM C140-96

Dry Density

189.3 pcf

ASTM C140-96

Bulk Specific Gravity

3.03

ASTM C140-96

Absorption

0.0%

ASTM C293-94

Modulus of Rupture

2,910 psi

ASTM C140-96

Compressive Strength

22,710 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

Mohs Hardness

7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

.728

.733

Polished

.594

.539

Thermal

.859

.754

Tapestry

.911

.846

Bush Hammer

.800

.900


Carmel Cream

Material Type: Quartzitic Sandstone

Material Class: Metamorphic

ASTM C97-96

Dry Density

145.8 pcf

ASTM C97-96

Bulk Specific Gravity

2.34

ASTM C97-96

Absorption

2.2%

ASTM C293-94

Modulus of Rupture

1,765 psi

ASTM C170-90

Compressive Strength

15,860 psi

ASTM C67-94

Freeze-Thaw Weight Loss

<0.5%

Mohs Hardness

6-7

ASTM C1028-89

Coefficient of Friction:

FINISH TYPE

DRY

WET

Sawn

.940

.806

Bush Hammer

1.000

1.060